TL;DR
Many industrial catalysts are tiny metal particles, a few nanometres across, held on a powdered oxide. A metal–support interaction is the change in the metal's behaviour caused by that oxide. In the strong form, the oxide partly migrates over the metal after the catalyst is heated in hydrogen, covering some of the metal's surface atoms. Fewer surface atoms are then available to bind reactant molecules, so the catalyst's activity and selectivity shift.
Builds on: Heterogeneous Catalysis, Nanoparticle, Redox Reaction, Chemisorption · Leads to: single-atom catalysts, and the design of supports for exhaust and fuel-processing catalysts
Where it's used
Automotive exhaust catalysts. A three-way catalyst converts carbon monoxide, unburnt fuel and nitrogen oxides in a car's exhaust, and it uses precious metals such as platinum, palladium and rhodium on oxides based on cerium dioxide. Ceria is a reducible oxide: it can gain and lose oxygen, which changes the oxidation state of its cerium ions, so the support can change its state in the hot, reducing and oxidising cycles of an engine. The engineers who tune these catalysts must allow for the interaction, because it affects how many metal atoms remain available to work.
Platinum on titanium dioxide. Titanium dioxide is a common support for platinum in studies of catalysis and photocatalysis. A standard finding is that, after reduction at a few hundred degrees Celsius in hydrogen, platinum takes up much less hydrogen and carbon monoxide than it did at lower temperatures. The metal is still there. Its surface has simply been partly covered.
Gold on oxides. Gold is inert as a bulk metal, but tiny gold particles on oxides such as titanium dioxide can catalyse the oxidation of carbon monoxide at low temperature. The support matters strongly for this activity, and the interaction between the gold and the oxide is a central part of why the particles work. Work on these systems followed the discovery around 1987 that small gold particles were active.
How it works
Take one tiny concrete case: a catalyst of platinum particles on titanium dioxide powder, measured in two states.
-
Start with clean platinum surfaces. Reduce the catalyst in hydrogen at about 200 degrees Celsius. The platinum particles are bare, and their surface atoms are free to bind hydrogen or carbon monoxide. Suppose 100 surface platinum sites are available. Check: the number of sites a molecule can bind to is the measure that the uptake test reports.
-
Raise the reduction temperature. Reduce the same catalyst in hydrogen at about 500 degrees Celsius. At this temperature the titanium dioxide surface loses some of its oxygen. The titanium ions drop to a lower oxidation state, so they are partly reduced, and the surface region becomes a mixed oxide that is no longer fully oxidised. Check: reduction removes oxygen from the oxide, which leaves it more reactive.
-
The reduced oxide spreads. The reduced oxide species become mobile at this temperature. They move across the support and onto the surface of the platinum particles, forming a thin layer over some of the metal atoms. Suppose this layer covers 25 of the 100 sites. Check: the layer sits on the metal, not beside it, so it sits on sites that were once free.
-
Electrons move at the interface. The reduced oxide and the metal exchange electrons, so the metal's electronic structure shifts near the contact. The metal surface becomes electron-rich there, and the bond between the metal and a reactant molecule changes. This is part of why the interaction changes the metal's chemistry, not just its coverage. Check: the change in the metal's behaviour is larger than the covered area alone would explain.
-
Measure the result. Hydrogen uptake now reflects only the exposed sites. Of the 100 sites, 75 remain bare, so the uptake falls to 75 percent of its original value. The catalyst is not destroyed, but its surface is different. Check: fewer bare sites means fewer molecules bound per gram, all else equal.
The visual below shows the sequence. The oxide that is reduced and mobile at high temperature is the cause of the covering.
flowchart LR A["Bare metal particles after low-temperature reduction"] --> B["High-temperature reduction of the oxide"] B --> C["Reduced oxide migrates onto the metal"] C --> D["Electrons shared across the interface"] D --> E["Fewer exposed metal sites and changed activity"]
The plot below shows how the exposed fraction of the metal falls as the covered fraction rises, which is the bookkeeping in step 5.
- exposed fraction = 1 - covered fraction
The math
A strong metal–support interaction (SMSI) is the state of a supported metal catalyst in which, after reduction at high temperature, a reducible oxide support covers part of the metal surface. The fraction of metal atoms that remain exposed is reduced, so chemisorption uptake falls below the value expected from the metal loading alone.
Step 1: counting sites
Let be the number of surface metal sites on the particles, and let be the number covered by oxide. The exposed sites are
and the exposed fraction is , where is the covered fraction. In step 3 of the walkthrough, and , so and .
Step 2: uptake in the chemisorption test
A chemisorption test measures how many molecules bind to the exposed sites. If each exposed site binds molecules, the uptake is . This is why the uptake falls by the same fraction as the exposed sites, provided each exposed site behaves as before.
Step 3: dispersion from uptake
The dispersion is the fraction of all metal atoms that sit on the surface. If the uptake is , the total metal is in the same units, and the stoichiometry is one molecule per surface atom, then
A drop in at fixed metal loading therefore gives a drop in . The electron transfer in step 4 of the walkthrough is not in this count, and it is the reason the activity can change even at the same dispersion.
Worked examples
- A catalyst has 100 exposed platinum sites before reduction at high temperature.
- After the oxide spreads, 25 sites are covered.
- The exposed sites are .
- The exposed fraction is .
- Interpretation: the metal has lost a quarter of its surface to the oxide. Uptake falls to 75 percent of the original, but none of the platinum has been removed.
Try it: the same catalyst, but now 40 of the 100 sites are covered. What is the exposed fraction? Answer: the exposed sites are , so the exposed fraction is .
- A catalyst takes up 100 micromoles of carbon monoxide per gram before high-temperature reduction, and 40 micromoles per gram after it.
- Compute the exposed fraction: .
- Compute the covered fraction: .
- Interpretation: sixty percent of the metal surface is covered by the oxide. If each exposed site behaves as before, the catalyst's rate per gram falls to about 40 percent of the earlier value.
- The assumption in step 4 is a real limit. The electron transfer in step 4 of the walkthrough can change the activity of the remaining sites as well, so the rate may fall by more or less than the uptake suggests.
- A catalyst contains 1 weight percent platinum, so 0.01 grams of platinum per gram of catalyst. The molar mass of platinum is 195.08 grams per mole.
- Compute the total platinum: moles, which is 51.3 micromoles per gram of catalyst.
- Before reduction at high temperature, hydrogen uptake is 20 micromoles per gram. Assuming one hydrogen per surface platinum atom, the dispersion is .
- After high-temperature reduction, uptake falls to 8 micromoles per gram. The dispersion is .
- Interpretation: about 39 percent of the platinum atoms were on the surface before the treatment, and about 16 percent after it. The change says the surface has been covered, and that the particles are still in place.
- Limits: the one-to-one stoichiometry is an assumption that varies with the metal, the gas and the temperature, so the numbers are a guide, not a certainty.
Try it: the same catalyst, now with uptake of 12 micromoles per gram after the high-temperature reduction. What is the dispersion? Answer: , so about 23 percent of the platinum is on the surface.
Common mistakes and tradeoffs
Mistake: "Low uptake means the metal is gone." It is tempting to think that a fall in hydrogen or carbon monoxide uptake means metal has been lost or sintered away. In fact the particles are still present, and the surface is partly covered by oxide. A measurement of the metal content, such as elemental analysis, will show the same amount of metal before and after.
Mistake: "The support is an inert shelf for the metal." It is tempting to think that the oxide only holds the particles apart. In fact a reducible oxide such as titanium dioxide or ceria can lose oxygen, change its state, and move onto the metal. Whether the support is inert or reducible therefore decides whether this interaction happens at all.
Mistake: "SMSI always makes a catalyst worse." It is tempting to think that covering the metal is a loss. In fact the covering can stabilise small particles against sintering, and it can change which products form, because the change in the metal's electron density alters the activation energy of competing routes. One product can then be favoured over another even when the products' thermodynamic stability is unchanged, because the choice is set by which route is faster. This is useful in some reactions. Whether it helps depends on the reaction.
When it matters. The interaction matters when the support is a reducible oxide and the catalyst is reduced at high temperature. It is important for designing long-lived exhaust catalysts, where the metal must stay dispersed for years.
When it does not. Supports such as silica and alumina are not easily reduced, and they show little of this effect. For those, uptake measurements track the metal's dispersion directly. Alternatives for controlling the interaction include choosing an inert support, lowering the reduction temperature, or adding a second metal.
History
Catalysts made of metal on oxide supports were used in industry long before their surfaces were understood at the atomic scale. For a long time, researchers assumed that a metal on an oxide acted as if the oxide were a passive base.
In 1978, S. J. Tauster and co-workers reported that noble metals on titanium dioxide lost much of their ability to take up hydrogen and carbon monoxide after reduction at high temperature. The effect was strong, it was not explained by simple sintering, and it was the reason the term strong metal–support interaction came into use.
Over the following years, electron microscopy and surface studies showed that the oxide could indeed form thin layers over the metal particles. The interaction was then studied in many oxides and metals, and it became a standard part of understanding how supported catalysts work. The later discovery that small gold particles on oxides were active for low-temperature carbon monoxide oxidation brought the support effect to wider attention.
Recap
- A catalyst metal particle on a reducible oxide can be partly covered by the oxide after high-temperature reduction.
- Covering the surface reduces the number of exposed sites, which lowers chemisorption uptake and the measured dispersion.
- The interaction also changes the metal's electron density at the contact, which can alter activity and selectivity beyond the covered fraction.
- Read next: single-atom catalysts push the idea of a supported metal to its limit, and density functional theory is one way to model the electron transfer at the interface.
Check yourself
QuestionA catalyst has 200 exposed metal sites before reduction and 150 after it. What fraction of the surface is covered by oxide?Show answer
The covered sites are , so the covered fraction is , or 25 percent of the surface.
QuestionWhy does a fall in chemisorption uptake not by itself prove that the metal has been lost from the support?Show answer
Uptake counts only the exposed metal sites that bind molecules. If the oxide covers some of the sites, uptake falls while all the metal is still on the support. Measuring the total metal content separately is needed to tell the two cases apart.
QuestionWhy is titanium dioxide more likely to show this interaction than silica?Show answer
Titanium dioxide is a reducible oxide: it can lose oxygen at high temperature, and its reduced species become mobile and spread over the metal. Silica is not easily reduced, so it does not form the mobile species that cover the metal.
QuestionA platinum catalyst has 0.02 grams of platinum per gram of catalyst. Its total platinum is about 102.5 micromoles per gram. If uptake falls from 30 to 15 micromoles per gram, what is the change in dispersion?Show answer
Before, the dispersion is . After, it is . The dispersion falls by about 0.15, from about 29 percent to about 15 percent.
QuestionWhy might a covered catalyst still be more useful than an uncovered one for some reactions?Show answer
The covering can keep small particles from merging into larger ones, which would lose surface area. It also changes the electron density of the remaining metal sites, which can favour some products over others. Whether this helps depends on the reaction and the desired product.